Main features

  • High reliability
  • High power applications
  • Good electrical performance

Product Description

Hysol GR600 SL2 is a halogen free, black, silica filled (87% filler weight) semiconductor grade epoxy molding compound designed for TO packages. This low stress, low moisture absorption product is a commercial success with many uses on TO applications.

Hysol GR600 SL2 is a green, heat curable epoxy molding compound that can be used in semiconductor packages such as TO252. Furthermore, it meets UL 94 V-0 flammability at 1/8 inch thickness.

Product Family

HYSOL GR600

1. Select Product Form
2. Select Pellet Size
3. Select Pellet Weight
4. Select Package Size
Catalog Product

Unlike other products we offer, the products listed on this page cannot currently be ordered directly from the website.

Product availability
US Shipping in 12 weeks
CA Shipping in 12 weeks
EU Shipping in 12 weeks
Packaging
Please select Product Form, Pellet Size, Pellet Weight and Package Size.
TDS, SDS & Technical Documents

Technical Specifications

General Properties
ColorColor
Black
Filler ContentFiller Content
87 %
Specific GravitySpecific Gravity
2.03
Electrical Properties
Volume ResistivityVolume Resistivity
14400000000000000 Ohms⋅cm
Chemical Properties
Moisture absorptionMoisture absorption
0.30 %
Physical Properties
Spiral Flow @ 175°CSpiral Flow @ 175°C
83 cm
Thermal Properties
Glass Transition Temperature (Tg)Glass Transition Temperature (Tg)
165 °C
Curing Conditions
Transfer PressureTransfer Pressure
40 - 85 kg/cm2
Transfer TimeTransfer Time
5 - 15 s

Leading Brands Trust in Our Products and Services

  • Jabil
  • Linxens
  • Magna
  • Medtronic
  • NXP
  • Philips
  • Semikron
  • Teledyne
  • Thales
  • Vishay
  • ZF
  • AMS
  • Apple
  • Audi
  • Broadcom
  • Borgwarner
  • Bosch
  • Eaton
  • Henkel
  • Honeywell
  • Hysol
  • Intel
Products that Perform|Knowledge that Serves|Service that Delivers